1. Summary

ABS (acrylonitrile–butadiene–styrene) is manufactured by combining a rubbery polybutadiene (PB) phase with a rigid styrene–acrylonitrile (SAN) matrix, and the industry's production technologies split along exactly that line.

Today two technology families dominate commercial production: continuous mass (bulk) polymerization, in which the rubber is dissolved in the monomers and polymerized in bulk, and the emulsion / hybrid route, in which the rubber is polymerized first as an aqueous polybutadiene latex, grafted with styrene and acrylonitrile in emulsion, recovered as a dry high-rubber powder, and then melt-blended with separately polymerized SAN resin. Versalis (Eni) states in its ONE-STEP® technology paper that "hybrid/emulsion technology accounts for about 97% of the ABS production globally"[1]; licensor patent backgrounds from PetroChina and Wanhua Chemical put the share of the dominant variant, emulsion grafting blended with bulk-polymerized SAN, at "80% or more" and "nearly 90% of suppliers" respectively[2][3].

This description covers the hybrid/emulsion family: its development lineage, the three-step process chain (latex synthesis and agglomeration, emulsion grafting and coagulation, blending and pelletizing), key operating parameters, the resulting product character compared with mass ABS, and the principal patents and technology packages behind it.


2. Development lineage

  • 1953–1966 — foundational emulsion graft patent. W. C. Calvert (Borg-Warner Corporation) filed US 3,238,275 (Sep 30, 1953; granted Mar 1, 1966) for polymerizing styrene–acrylonitrile monomer mixtures directly in an aqueous polybutadiene latex — the graft reaction that converts a rubber latex into an impact-modified ABS resin and the basis of the emulsion route[4]. Early commercial ABS was in fact produced in emulsion; mass polymerization entered commercial use only from the mid-1980s[7].
  • 1950s–1970s — latex morphology development. Monsanto (later Bayer Antwerpen) patented the bimodal rubber-latex concept (US 4,385,157, filed Nov 27, 1981), in which a small-particle PB latex mode is formed first and additional emulsifier creates a second, smaller mode before grafting, giving ABS polyblends a bimodal rubber particle size distribution with high impact at small average particle size[5].
  • 1970s–2010s — the hybrid route consolidates. The combination "emulsion grafting + separately produced bulk SAN + melt blending" became the dominant global route. China's first ABS line (Lanzhou Petrochemical, 1975, 2 kt/a) used synthetic-rubber emulsion grafting, and Chinese producers subsequently standardized on the emulsion-graft–bulk-SAN blending variant[8] (see the China cleaner-production case study and CNPC packaged-technology sources below). CNPC now offers the route as a complete "Packaged ABS Resin Technology"[8].
  • 2007–2023 — the mass-route counterpoint. Versalis (Polimeri Europa) developed the ONE-STEP® integrated anionic/radical process (WO 2009/074244, priority Dec 12, 2007) to bring "emulsion-like" rubber particle sizes to the continuous mass route, explicitly positioning the mass process against the 97% hybrid/emulsion incumbent[1][6].
  • 2010s–2020s — continuous upgrades. Chinese producers continue to patent refinements of the hybrid route: full-continuous latex-graft–coagulation–blending lines (CN 103193940A, 2012), coagulant and kettle-plus-tube coagulation improvements (CN 112876586B, Wanhua, 2021), methyl-methacrylate third-stage polymerization to cut residual monomers (CN 111171239A, PetroChina, 2018) and whiter graft-powder coagulation (CN 105601769A, Tianjin Dajie, 2016)[2][3][9][10].

3. Process overview

The hybrid/emulsion family divides ABS synthesis into two independent production trains that meet only at the final compounding step. This separation is the source of both its flexibility (rubber content, particle size and SAN molecular weight are adjusted by changing the blend ratio rather than the polymerization itself) and its longer flowsheet compared with mass ABS[1][2][8].

Section Function Typical documented conditions
PB latex synthesis Emulsion polymerization of butadiene (with a small styrene fraction) to small-particle rubber latex 40–80 °C continuous synthesis (CN 103193940A); 80–120 nm particles (CNPC two-stage route)[9][8]
Chemical agglomeration Grows small-particle PB latex to the target grafting particle size (bimodal distributions possible) 17–60 °C (CN 103193940A); 120–400 nm final particle size, agglomeration <1 h (CNPC)[9][8]
Emulsion grafting Graft copolymerization of styrene and acrylonitrile onto the PB latex (graft shell around the rubber core) 30–80 °C (CN 103193940A); rosin-soap emulsifier, redox initiator, 50→65→75 °C stages, graft-powder rubber content 40–75%, conversion >98%[2][9]
Coagulation Breaks the graft latex emulsion into ABS graft powder slurry (acid/salt coagulants) ~75 °C flocculation + ~95 °C ripening, three continuous stirred coagulators most common; sulfate coagulants (H2SO4/MgSO4) typical[3]
Dewatering and drying Centrifugal dewatering and fluidized-bed drying of the wet graft powder Nitrogen-circulating fluidized bed, moisture <1% (CNPC)[8]
Continuous bulk SAN synthesis Thermally initiated continuous bulk copolymerization of styrene and acrylonitrile; two-stage devolatilization 55–65% polymer solids at discharge, ~70% conversion, monomer/solvent recycled (CNPC)[8]
Melt blending and pelletizing ABS graft powder + SAN pellets + additives fed to twin-screw extrusion and pelletizing 200–250 °C continuous extrusion (CN 103193940A); powder:SAN blend ratios (20:80)–(30:70) at 200–230 °C in patent examples[9][2]

4. Step-by-step process description

4.1 Polybutadiene latex synthesis

Butadiene monomer is polymerized in water with a compound emulsifier system, molecular-weight regulator and inorganic peroxide initiator under agitation. Chinese industrial practice (CNPC packaged technology) runs this first stage to small-particle latex of 80–120 nm, with short polymerization times, conversion high enough that no butadiene recovery section is needed, and latex stability sufficient for more than two years of storage[8]. The Monsanto bimodal process shows the alternative single-reactor approach: butadiene is polymerized to 5–50% conversion with an initial emulsifier charge to form a 0.2–0.5 µm particle mode, then a second emulsifier addition creates a second, smaller mode before polymerization is driven to 70–100% conversion[5].

4.2 Particle-size build-up (agglomeration)

Small-particle PB latex is chemically agglomerated to the particle size required by the target ABS grade — CNPC cites 120–400 nm trunk latex for grafting, with agglomeration times under one hour and latex precipitation below 0.03%[8]. The continuous patent route specifies agglomeration at 17–60 °C[9]. Particle size, distribution, pH and viscosity are the control parameters that determine final impact strength and surface gloss; for high-impact ABS, PB latex particle sizes of roughly 290–350 nm are reported as typical industrial targets[2].

4.3 Emulsion grafting of styrene and acrylonitrile

Styrene and acrylonitrile are added to the agglomerated PB latex and copolymerized in emulsion. Part of the monomer grafts onto the rubber particles (forming the SAN shell that compatibilizes rubber and matrix) while the remainder forms free SAN matrix polymer; the graft-to-matrix balance is set by the monomer-to-rubber ratio, emulsifier level, initiator system and addition schedule[5][2]. Published patent examples use rosin-acid-soap emulsifiers, redox initiation (cumene hydroperoxide or persulfate with ferrous sulfate activators), tertiary-dodecyl-mercaptan chain-transfer agent and staged temperatures of 50 °C, 65 °C and 75 °C across successive monomer additions, with total reaction times of a few hours and graft-powder rubber contents of 40–75 wt%[2][8]. High graft conversion (>98%) is a stated design objective because unreacted monomer in the graft powder, not in the SAN, dominates residual monomer in the final resin[2].

4.4 Coagulation, dewatering and drying

The graft latex is destabilized with acid/salt coagulants — sulfuric acid with magnesium sulfate being the most common industrial pair — in a coagulation train typically consisting of a low-temperature flocculation stage (~75 °C) followed by high-temperature ripening (~95 °C), most often in three continuous stirred-tank reactors[3]. The slurry is cooled, filtered or centrifuged to a wet graft powder, and dried in nitrogen- or air-circulating fluidized beds; CNPC's packaged technology specifies a nitrogen fluidized bed holding powder moisture below 1% for safety with flammable powder[8]. Coagulation chemistry is a live optimization area: residual metal ions from sulfate coagulants promote yellowing during subsequent drying and melt blending, and recent patents propose metal-free coagulant systems (for example 1,2,4,5-benzenetetramine tetrahydrochloride with EDTA tetrasodium, combined with a kettle-plus-tube serial continuous coagulation to narrow the powder size distribution)[3].

4.5 Bulk SAN synthesis

Styrene and acrylonitrile are copolymerized continuously in bulk (thermal initiation, optional solvent), discharged at 55–65% polymer solids and roughly 70% conversion, then devolatilized in two stages — acrylonitrile removed at lower temperature in the first stage to limit yellowness, styrene removed at higher temperature and vacuum in the second — with recovered monomer recycled to polymerization. The SAN is pelletized (underwater or strand granulation) for blending[8]. Because this SAN train is shared conceptually with continuous mass ABS, the same reaction hardware family serves polystyrene, HIPS and SAN, making it a flexible multi-product asset [9].

4.6 Melt blending and pelletizing

ABS graft powder and SAN pellets are proportioned continuously and compounded with additives (antioxidants, lubricants, colorants) on twin-screw extruders, then pelletized. Published blend windows are graft-powder-to-SAN ratios of (20:80)–(30:70) at 200–230 °C[2], and the fully continuous patent route specifies blending and extrusion at 200–250 °C[9]. The blend ratio — not the polymerization recipe — is the principal grade-switching lever, which is why the route covers the widest commercial ABS portfolio, from high-gloss general-purpose to high-impact, high-heat, electroplatable and flame-retardant grades[1][8].


5. Product characteristics: hybrid/emulsion ABS versus mass ABS

  • Rubber morphology. Emulsion ABS has smaller, full (non-occluded) rubber particles; mass ABS particles are larger and formed by in-situ phase inversion, constrained by the viscosity ratio achievable in bulk[1]. The bimodal latex distributions achievable in emulsion give high impact at small average particle size[5].
  • Surface and colour. The hybrid/emulsion route produces glossy ABS, which Versalis notes is "preferred in the marketplace in contrast to a matte finish provided by mass ABS"[1]. Mass ABS offers a consistent light base colour and matt or dull surfaces valued in automotive interiors but not in most consumer appliance or electrical/electronic applications[1].
  • Economics and environment. The mass process has lower utility and fixed costs than the hybrid/emulsion process; for the comparable route, the bulk route's investment was reported about 45% lower and total production cost about 8% lower (2012 levels), with lower material and energy consumption and minimal effluent — at the cost of narrower grade flexibility, rubber content generally below ~20% and lower gloss[1] [9].
  • Grade flexibility. Adjusting graft-powder/SAN blend ratios lets producers switch quickly between high-impact, high-gloss, high-heat and specialty grades, the key commercial reason the hybrid/emulsion route holds the overwhelming majority of global capacity[1][2][8].

6. Comparative economic performance

Versalis states that "the mass process is actually lower in production cost than the hybrid/emulsion process due to lower utility and fixed costs"[1]; the Chinese G-vs-B comparison at 2012 levels quantifies the same direction (investment ~45% lower, total cost ~8% lower for mass), while noting the mass route's product limitations [9]. No independent third-party same-basis economic study comparing the two routes across current global assets was located in the reviewed public sources; the figures above are licensor- and trade-press-declared.


7. Commercial experience and technology packages

  • Scale. The hybrid/emulsion family accounts for the large majority of world ABS capacity: about 97% of global ABS production per Versalis[1], "80% or more" of total output for the emulsion-graft + bulk-SAN blending variant per PetroChina's patent background[2], and "nearly 90% of suppliers" using that route per Wanhua[3]. The continuous mass route was reported at roughly 15–20% of output (2017) [9].
  • Producers on the hybrid/emulsion route. Large Asian ABS producers operate emulsion-graft–bulk-SAN blending lines, including CHIMEI (Taiwan and Zhenjiang) and LG Chem, with Chinese producers (CNPC/PetroChina bases, Wanhua Chemical's Yantai/Penglai complex with a 200 kt/a ABS project, Tianjin Dajie and others) continuing to expand on this route[2][3][8]. PetroChina's first line (Lanzhou, 1975) established the route in China [8].
  • Technology packages. CNPC markets a complete "Packaged ABS Resin Technology" covering the full emulsion-graft + bulk-SAN line: small-particle PB polymerization, chemical agglomeration, graft polymerization, continuous three-reactor coagulation, nitrogen drying, SAN bulk polymerization with two-stage devolatilization, continuous proportioning/mixing and granulation[8]. On the mass side, Versalis licenses the ONE-STEP® integrated process (WO 2009/074244 family; EP 2222741B1, US 8404781B2, CN 101910226B) to produce "emulsion-like" mass ABS[1][6].
  • Residual-monomer control. Emulsion graft powder is the main residual-monomer carrier in final ABS (residual monomer in graft powder reported above 3,000 ppm vs SAN below 1,000 ppm after vacuum devolatilization); PetroChina's staged third-monomer approach is one published countermeasure[2].

8. Key patents

Patent / family Priority Subject
US 3,238,275 A (Calvert, Borg-Warner) 1953-09-30 (granted 1966-03-01) Polymerization of styrene–acrylonitrile mixtures in polybutadiene latex — foundational emulsion-graft ABS process [4]
US 4,385,157 A (Auclair & Paul, Monsanto) 1981-11-27 (granted 1983-05-24) Bimodal PB latex emulsion grafting for ABS polyblends [5]
WO 2009/074244 A1 (Polimeri Europa / Versalis; EP 2222741B1, US 8404781B2, CN 101910226B) 2007-12-12 ONE-STEP® integrated anionic rubber synthesis + solvent exchange + continuous mass ABS — the mass-route counterpart [6]
CN 103193940 A (Li Yishan) 2012-01-10 Fully continuous, high-safety emulsion-graft blending ABS process with documented temperature windows [9]
CN 111171239 A (PetroChina) 2018-11-09 Staged emulsion grafting with methyl-methacrylate third stage to cut residual monomers; blend-ratio and temperature examples [2]
CN 112876586 B (Wanhua Chemical) 2021-01-18 (granted 2022-11-08) Metal-free coagulant system + kettle-plus-tube serial continuous coagulation for ABS graft latex [3]
CN 105601769 A (Tianjin Dajie Chemical) 2016-03-03 Graft-latex coagulation method improving ABS base colour (SFS system) [10]

9. Notes

  • Share-of-production figures differ by source and basis. Versalis reports hybrid/emulsion technology at about 97% of global ABS production[1]; PetroChina's patent background puts emulsion grafting + bulk SAN blending at "about 80% or more" of total output[2]; Wanhua states "nearly 90% of suppliers" use that route[3]; a 2017 Chinese trade review put continuous mass at roughly 15–20% of output [9]. All are licensor/author-declared; no independent audit of global route shares was located.
  • Terminology. "Hybrid/emulsion" as used here covers emulsion grafting combined with separately produced SAN (the emulsion-graft + bulk-SAN blending variant being dominant); pure emulsion-graft with emulsion-SAN blending has been phased out in developed markets, and the suspension-SAN variant is niche [9].
  • Comparators. The continuous mass (bulk) route — described in detail in ppPLUS companion profiles and in Versalis' ONE-STEP® literature — is covered here only to the extent needed to delimit the hybrid/emulsion family[1][6].

10. References

  1. Versalis (Eni) — Gavioli S., Chiezzi L., Inglese R., Leone M.A., ABS ONE-STEP® Technology — Major Improvements in Versalis' Proprietary ABS Continuous Mass Process, Chemical Engineering Transactions, vol. 100, pp. 451–456, DOI:10.3303/CET23100076 (Jun 9, 2023; received Feb 15, 2023; accepted Jun 9, 2023; PDF also in task folder)
  2. PetroChina Co., Ltd. — ABS Resin and Preparation Method Thereof, CN 111171239A (filed Nov 9, 2018; published May 19, 2020)
  3. Wanhua Chemical Group Co., Ltd. / Wanhua Chemical (Sichuan) Co., Ltd. — Coagulation Method for ABS Graft Latex, CN 112876586B (filed Jan 18, 2021; granted Nov 8, 2022)
  4. Calvert, W. C. (Borg-Warner Corporation) — Polymerization of Acrylonitrile-Styrene Mixtures in the Presence of Polybutadiene, US 3,238,275 A (filed Sep 30, 1953; granted Mar 1, 1966)
  5. Auclair, R. M.; Paul, R. (Monsanto Company) — Emulsion Polymerization Process for ABS Polyblends, US 4,385,157 A (filed Nov 27, 1981; granted May 24, 1983)
  6. Inglese, R.; Chiezzi, L.; Montanari, F.; Casalini, A. (Polimeri Europa S.p.A.) — Semi-continuous Integrated Process for the Production of High Impact Vinyl Aromatic (Co)polymers by Anionic/Radical Polymerization in Sequence, WO 2009/074244 A1 (priority Dec 12, 2007; published Jun 18, 2009)
  7. Li Yishan — Production Process for ABS Resin, CN 103193940A (filed Jan 10, 2012; published Jul 10, 2013)
  8. China National Petroleum Corporation, Science & Technology Management Department — Packaged ABS Resin Technology (2011; PDF created Nov 10, 2011)
  9. Ronton Plastics Media — Bulk ABS Resin Industry Status and Technology Innovation (Jan 4, 2017)
  10. Tianjin Dajie Chemical Co., Ltd. — Graft Latex Coagulation Method for Improving the Base Colour of ABS Resin, CN 105601769A (filed Mar 3, 2016)

Insight Articles
Your insights will be shown here

No entries
Title Date
Technology Owner Entity
Content provided by
Transaction Name Date
Modified by UserPic   Kokel, Nicolas 11/18/2026 4:53 PM
Added 11/18/2026 3:33 PM